Hey again, when i’m glassing is it alright for fiberglass to overlap each other? and how much catalyst should i use for one quart of resin? thanks
At 75º try about 10 ml. At 85º about 8 ml. This is kind of slow so you should have plenty of work time. The fiberglass is supposed to lap over itself. When you laminate, have about a 2" overlap hanging. When you wet the lap the glass will then stick to the other side when you sqeegee it under. After it kicks you sand that lap so the second side glass will go smoothly over. On laminating the second side you follow the same method as the first with the same kind of overlap.
alrite thanks alot. I’m gonna go glass now, hopefully it’ll turn out alrite thanks again!